TN-02 2 min read Barrier Packaging
When oxygen transmission rises in an EVOH laminate
Humidity, local thinning and delamination call for different measurements. A single oxygen transmission rate cannot distinguish them.
The humidity behind the reported value
Zhang, Britt and Tung varied relative humidity and temperature in tests on EVOH films. Above 75% relative humidity, permeability rose substantially in their specimens. Ethylene content and orientation also affected the result. The reported humidity belongs to that experiment. In a laminate, the surrounding layers and conditioning time also affect how much moisture reaches the EVOH.
Control the sample history
For a PE/tie/EVOH/tie/PE structure, cut paired specimens from the same roll. Record conditioning time, temperature, humidity on each side during measurement and which face was exposed to the humid stream. Compare steady readings at the same oxygen partial-pressure difference. For a formed tray, take sections at the wall and corner to check the remaining barrier thickness before comparing it with flat sheet.
Test the suspect interface separately
If oxygen transmission rises, inspect the specimen for pinholes and local thinning. On adjacent specimens, examine the cross-section and, where a layer can be isolated, test adhesion after the same conditioning. A change in permeation with a stable peel result gives a different lead from visible separation along one interface. Neither observation alone identifies the cause.